Elektra92 (AR-PC-5090)
Tone | Conductive Polymer |
Reference | All resist: https://www.allresist.com/portfolio-item/protective-coating-ar-pc-5090-02-electra-92/ |
Spin coat | After spincoating and baking your resist spincoat elektra92: 2000 rpm: 60 nm (See datasheet manufacturer) |
Prebake | 900C, 2 minutes on hotplate or 850C , 25 minutes in oven |
Exposure | According to your image layer |
Removal elektra92 | Remove after exposure before you develop your image layer as follows: DI water for 2 minutes at 400C or ultrasonic as needed |
Development | According to your image layer |
Rinse | According to your image layer |